VT-441 Laminate/Prepreg
UL Approval: E214381 Version: C1 27/04/2020 /127/128General Information
- Phenolic Cured System
- Halogen free & Mid-Tg FR4.1
- UV Blocking
- CAF Resistance
- Low Z-CTE
- Excellent Thermal Reliability
Application
Mobile Phone, Smart Phone, Computer, Instrumentation, Communication Equipment, Electronic Game Machine, VCR, etc.
Availability
- Core Thickness: 0.002” (0.05mm) to 0.200” (5mm), available in sheet or panel form
- Copper Foil: 1/4oz to 12oz
- Prepregs are available in roll or panel form
- E-Glass styles: 7628, 1506, 1500, 2113, 2313, 3313, 2116, 1080, 1086, 1078, 106 & 1067, etc.
Note: For cores ≤ 0.005”, it is recommended to use the reverse treated copper due to the low profile. The peel strength for RT foil is ≈1-2lbs/in (0.35Kg/m) less than standard foil.
Properties Prepreg Laminate Storage Condition Temperature Below 23°C (73°F) Below 5°C (41°F) Room Relative humidity Below 55% RH / / Shelf Life 3 months 6 months 24 months (airproof) The prepreg exceeding shelf life should be retested.
Properties Sheet IPC-4101E /127 /128
Properties Test Method Units Specification Typical Value Thermal Properties Tg DSC IPC-TM-650 2.4.25 °C 150 minimum 152 TMA IPC-TM-650 2.4.24 °C 150 minimum 158 Td ASTM D3850 °C 325 minimum 385 T260 IPC-TM-650 2.4.24.1 Minute 30 minimum >60 T288 IPC-TM-650 2.4.24.1 Minute 5 minimum >30 Thermal Stress @ 288°C IPC-TM-650 2.4.13.1 Second Pass 10s >600 Z-axis CTE Before Tg IPC-TM-650 2.4.24 ppm/°C 60 maximum 38 After Tg IPC-TM-650 2.4.24 ppm/°C 300 maximum 190 Total Expansion (50~260°C) IPC-TM-650 2.4.24 % 3.5 maximum 2.2 X-Y CTE IPC-TM-650 2.4.24 ppm/°C - 11~13 MOT UL 94 °C - 130 Electrical Properties DK @ 1GHz RC 50% IPC-TM-650 2.5.5.9 - 5.4 maximum 4.4 DF @ 1GHz RC 50% IPC-TM-650 2.5.5.9 - 0.035 maximum 0.014 Volume Resistivity After Moisture Resistance IPC-TM-650 2.4.17.1 MΩ-cm 1.0E+4 minimum 5.0E+8 E-24/125 IPC-TM-650 2.4.17.1 MΩ-cm 1.0E+3 minimum 5.0E+6 Surface Resistivity After Moisture Resistance IPC-TM-650 2.4.17.1 MΩ 1.0E+4 minimum 5.0E+7 E-24/125 IPC-TM-650 2.4.17.1 MΩ 1.0E+3 minimum 5.0E+6 Electrical Strength IPC-TM-650 2.5.6.2 Volt/mil (KV/mm) 762 (30) minimum 1200~1400 (54) Dielectric Breakdown IPC-TM-650 2.5.6 KV 40 minimum 60 Comparative Tracking Index (CTI) ASTM D3638 Rating (Volt) - Grade 3 (175~250) Arc Resistance ASTM D495 Second - 187 Mechanical Properties Peel Strength (1oz) As received IPC-TM-650 2.4.8 lb/in (N/mm) - 7~9 (1.2~1.6) After thermal stress IPC-TM-650 2.4.8 lb/in (N/mm) 6 (1.05) minimum 7~9 (1.2~1.6) Flexural Strength Warp IPC-TM-650 2.4.4 KPsi (MPa) 60 (415) minimum 72 (500) Fill IPC-TM-650 2.4.4 KPsi (MPa) 50 (345) minimum 58 (400) Physical Properties Moisture Absorption IPC-TM-650 2.6.2.1 % 0.80 maximum 0.18 Flammability UL-94 Rating V-0 minimum V-0 All test data provided are typical values and not intended to be specification values. Disclaimer: The information and data contained in this technical literature is based on data and knowledge correct at the time of publishing/printing and is believed to be accurate and is offered in good faith for the benefit of the user. The user should make his own tests to verify the suitability of this product for any application before its use. All data are typical values only and subject to change without notice.
Published on: 27/04/2020
-
VT-441 CCL/Laminate VT-441 PP/Prepreg
UL Approval: E214381 Version: Rev. B4 24/06/2018 /127/128Storage Condition & Shelf Life
Precautions In Handling
- The prepreg exceeding shelf time should be retested.
- Take care in handling thin core laminates as they are easily damaged.
- If the prepreg is not consumed within 48hrs after opening the vacuum package, it is recommended that the bags be resealed.
- Material is available in both long and short grain. The grain direction is indicated on the label with an arrow.
Designing And Inner Layer Process
- Please be careful when single ply of 1080, 1086, 1078 or 106 prepreg is designed to the dielectric layer.
- Dimension stability is the same as Standard FR4 material.
- Please check with your oxide vendor to make sure that our material is suitable with your oxide process. We recommend to control the peel strength with brown oxide copper over 2 Lb/in.
- For unclad or single sided laminates to be used in multilayer, please brush unclad sides before use.
Prepreg Availability
E-Glass styles: 7628, 1506, 1500, 2113, 2313, 3313, 2116, 1080, 1086, 1078, 106, 1067 etc.Prepreg Availability
PP Type Resin Content Press Thickness (mil) DK DF Remark @ 1GHz @ 2GHz @ 5GHz @ 10GHz @ 1GHz @ 2GHz @ 5GHz @ 10GHz 7628 45% 7.50 4.35 4.30 4.25 4.25 0.012 0.013 0.013 0.014 Standard 1506 52% 7.20 4.15 4.10 4.05 4.05 0.013 0.014 0.014 0.015 Standard 2116 58% 5.20 3.98 3.93 3.88 3.88 0.013 0.014 0.014 0.015 Standard 2116 54% 4.70 4.10 4.05 4.00 4.00 0.013 0.014 0.014 0.015 Standard 2116 52% 4.50 4.15 4.10 4.05 4.05 0.013 0.014 0.014 0.015 Standard 2113 57% 4.10 4.00 3.95 3.90 3.90 0.013 0.014 0.014 0.015 Standard 1080 68% 3.20 3.80 3.73 3.68 3.68 0.014 0.015 0.015 0.016 Standard 1080 66% 3.00 3.83 3.76 3.70 3.70 0.014 0.015 0.015 0.016 Standard 1078 65% 3.00 3.83 3.76 3.70 3.70 0.014 0.015 0.015 0.016 Standard 1067 73% 2.70 3.72 3.62 3.56 3.56 0.015 0.016 0.016 0.017 Standard 106 76% 2.30 3.68 3.58 3.50 3.50 0.016 0.017 0.017 0.018 Standard 1037 72% 2.00 3.77 3.68 3.63 3.63 0.015 0.016 0.016 0.017 Standard ① Press thickness test condition---Prepreg lamination size 18”*24”, Copper Foil---1oz/1oz, Flow---about 5%; ② Make laminated prepreg to micro-section and measure the thickness with microscope; this thickness is used for resistance design calculation. ③ The thickness measured with micrometer is 0.2~0.4 mil larger than that measured with micro-section; and mainly used for total thickness design calculation.
Laminate Availablity
Thickness: 0.002” (0.05mm) to 0.200” (5mm), available in sheet or panel form Copper Foil: 1/4 to 12oz, HTE or RTF or DST DK values are for impedance design.Laminate Availability
Core thk. (Inches) Stack-up Resin Content DK DF Remark @ 1GHz @ 2GHz @ 5GHz @ 10GHz @ 1GHz @ 2GHz @ 5GHz @ 10GHz 0.0015 1-1027 70% 3.77 3.67 3.60 3.60 0.015 0.016 0.016 0.017 Standard 0.002 1-1037 72% 3.73 3.63 3.58 3.58 0.015 0.016 0.016 0.017 Non-standard 0.002 1-106 72% 3.73 3.63 3.58 3.58 0.015 0.016 0.016 0.017 Standard 0.003 1-1080 66% 3.83 3.73 3.68 3.68 0.014 0.015 0.015 0.016 Standard 0.004 1-2116 46% 4.35 4.30 4.25 4.20 0.013 0.014 0.014 0.015 Standard 0.004 2-106 72% 3.73 3.63 3.58 3.58 0.015 0.016 0.016 0.017 2ply 0.005 1-2116 55% 4.05 4.00 3.95 3.95 0.013 0.014 0.014 0.015 Standard 0.006 1-1506 45% 4.35 4.30 4.25 4.20 0.012 0.013 0.013 0.014 Standard 0.007 1-7628 41% 4.50 4.45 4.40 4.40 0.012 0.013 0.013 0.014 Standard 0.008 1-7628 46% 4.35 4.30 4.25 4.25 0.012 0.013 0.013 0.014 Standard 0.008 2-2116 46% 4.35 4.30 4.25 4.25 0.012 0.013 0.013 0.014 2ply 0.010 2-2116 55% 4.05 4.00 3.95 3.95 0.013 0.014 0.014 0.015 Standard 0.012 2-1506 45% 4.35 4.30 4.25 4.25 0.012 0.013 0.013 0.014 Standard 0.014 2-7628 41% 4.50 4.45 4.40 4.40 0.012 0.013 0.013 0.014 Standard 0.016 2-7628 46% 4.35 4.30 4.25 4.25 0.012 0.013 0.013 0.014 Standard 0.028 4-7628 41% 4.50 4.45 4.40 4.40 0.012 0.013 0.013 0.014 Standard 0.036 5-7628 43% 4.40 4.35 4.30 4.30 0.012 0.013 0.013 0.014 Standard 0.045 6-7628 46% 4.35 4.30 4.25 4.25 0.012 0.013 0.013 0.014 Standard 0.049 7-7628 41% 4.50 4.45 4.40 4.40 0.012 0.013 0.013 0.014 Standard 0.059 8-7628 44% 4.40 4.35 4.30 4.30 0.012 0.013 0.013 0.014 Standard Press Condition
1. Heating rate(Rise of Rate) of material [Material Temperature]
Programmable Press: 1.5-3.0℃/min (3~5℉/min). Manual Press:3~6℃ /min (5~10℉/min)2. Curing Temperature & Time: >50min at more than 180℃ (356℉)[Material Temperature]
3. Full Pressure : ≥250-300psi
4. Vacuuming should be continued until over 140℃ (284℉) [Material Temperature]
5. Cold Press condition:
Keep Plate @ Room Temperature by water, Pressure:100psi, Keep Time:60minutesTypical Drilling Parameters (φ0.3-1.0 mm)
Desmearing Process
1. Desmear rate of VT-441 is less than that of the conventional FR4; 2. Adjustments to the desmear process are necessary for the lead-free materials; 3. Check with your chemical supplier for recommendations.